How to repair cracks in brick walls

Learn how to repair cracks in brick walls using Australian standards. Fix mortar joints, replace fractured bricks, and identify structural foundation movement.

Quick answer

Repair cracks in brick walls by raking out damaged mortar to a depth of 15 to 20 millimetres, dampening the joint, and repointing with a matching cement-lime sand mortar. Fractured bricks must be removed and replaced. Cracks exceeding 5 millimetres require a structural engineer under AS 2870.

Skill level
Intermediate
Time
4–8 hours for minor repairs, 1–2 days if replacing damaged bricks and allowing for curing
Trade
Building & Construction
Updated
29 November 2026

Tools you will need

  • Makita 125mm SJSII Angle Grinder with Dust Extraction Shroud
  • Carbide Mortar Raking Bit 8mm or Diamond Pointing Blade
  • Ox Tools Pro Heavy Duty Plugging Chisel
  • Marshalltown 125mm London Style Pointing Trowel
  • Selleys 420g Heavy Duty Caulking Gun
  • Stabila Type 196-2 Heavy Duty 1200mm Spirit Level
  • Hilti VC 20-U M-Class Dust Extractor Vacuum

🧱 How to Repair Cracks in Brick Walls

What is involved in repairing cracks in brick walls?

Repairing cracks in brick walls depends on whether the damage is cosmetic in the mortar joints or a sign of structural movement in the masonry itself. For Australian homeowners, small stable cracks can often be repaired with repointing, brick replacement, or flexible sealants, but wider or progressing cracks should be assessed by a structural engineer or licensed bricklayer in line with AS 3700 Masonry Structures and local council requirements.

What skill level is required to repair brick wall cracks in Australia?

Intermediate — Estimated time: 4–8 hours for minor repairs, 1–2 days if replacing damaged bricks and allowing for curing

What tools are essential for repairing brick wall cracks?

Brick bolster and club hammer for cutting out mortar and removing damaged bricks
Angle grinder with 100 mm–125 mm diamond masonry blade for raking joints
Plugging chisel for controlled mortar removal
Pointing trowel and brick trowel
Jointing tool or tuck pointer to match existing mortar profile
Stiff masonry brush and hand broom
Bucket for mixing mortar
Mortar mixing drill with paddle, or cement mixer for larger repairs
Spray bottle or garden sprayer for dampening brickwork
Caulking gun for masonry crack sealant where applicable
Spirit level and straightedge for checking wall alignment
Tape measure
Ladder or compliant scaffold for work at height
PPE: safety glasses, dust mask or P2 respirator, hearing protection, gloves, steel-cap boots

What materials are needed for brick wall crack repair?

Mortar mix matched to existing wall colour and strength
General repair mortar using 1:2:3 cement:lime:sand where suitable for common masonry repairs
Washed brickies sand
Clean water
Replacement bricks matched in size, colour and texture if any bricks are split or loose
Masonry crack filler or paintable polyurethane sealant for very fine non-structural cracks
Bond breaker or foam backer rod for wider non-structural gaps if sealing
Brick ties or helical repair bars only where specified by an engineer or repair system manufacturer
Oxide colour additive if required for mortar colour matching
Plastic sheeting or hessian for curing protection
Mild brick cleaning solution if final cleanup is needed

Safety Requirements

Wear safety glasses, gloves, hearing protection and a P2 dust mask when grinding or chiselling masonry.
Silica dust from bricks and mortar is hazardous; use dust suppression and avoid dry cutting where possible.
Use correct manual handling when lifting bricks, mortar bags and equipment.
If working above ground level, use stable access equipment and compliant scaffolding where required.
Do not repair significant structural cracks without professional assessment; stepped cracking, bulging walls, or cracks wider than 5 mm may indicate footing failure or structural movement.
Any structural repair should be designed or certified by an engineer and may require compliance with state regulations and council approval.
Check for buried services, electrical conduits or plumbing if working near wall penetrations.

Step-by-Step Guide

Step 1: Inspect the crack and determine the cause

Start by identifying the type of crack. Hairline cracks in mortar joints are usually cosmetic, while diagonal or stepped cracks following the mortar joints can indicate movement from footings, reactive soil, tree roots, storm events, or moisture changes.

Measure the crack width. As a general guide:

Hairline to 1 mm: usually cosmetic
1–5 mm: minor movement or mortar deterioration
Over 5 mm: possible structural issue requiring expert assessment

Look for warning signs such as doors or windows sticking, wall bulging, bricks pushed out of line, fresh cracking after rain or drought, or gaps reopening after previous repair. If the crack is actively moving, repairing it without fixing the cause will only be temporary.

💡 If you are unsure whether the crack is still moving, mark both ends with pencil and date them, or use a simple crack monitor over several weeks.

Step 2: Decide whether it is a DIY repair or a job for a professional

DIY repair is generally suitable where:

The crack is minor and stable
Damage is limited to mortar joints
Only one or two bricks are chipped, loose or lightly cracked
There is no wall bulging or foundation movement

Call a licensed bricklayer, builder or structural engineer if:

Cracks are wider than 5 mm
The wall is leaning, bulging or separating
The crack runs through multiple courses and keeps growing
It affects a loadbearing wall, retaining wall or wall supporting a roof
There is storm, vehicle or impact damage
Internal and external cracks line up through the wall

Structural crack stitching systems, underpinning and footing repairs should be completed to an engineered specification, with reference to AS 3700 and, where relevant, AS 2870 Residential slabs and footings.

Step 3: Prepare the work area

Clear the area around the wall and protect nearby paving, windows, plants and finishes with drop sheets. If the wall is painted or rendered, note that the repair process differs and may need additional surface restoration.

Use a stiff brush to remove dirt, salts and loose material around the crack. For mortar repairs, rake out the cracked joint to a depth of at least 15–20 mm, or roughly 2 times the joint width, until you reach firm material.

An angle grinder can speed up the job, but use care not to damage the brick arrises. For small repairs, a plugging chisel and hammer give better control.

💡 Always remove enough loose mortar to give the new repair mortar something solid to key into. Thin smears over the surface will fail quickly.

Step 4: Repair fine non-structural cracks

For very fine, stable cracks less than about 2 mm, especially where they are in mortar or at interfaces, a masonry crack filler or high-quality paintable exterior polyurethane sealant can be used.

Open the crack slightly if required by the product instructions, remove dust, and lightly dampen the area if recommended. Apply the filler evenly with a caulking gun, then tool it off neatly so it sits flush with the joint.

This method is best for small cosmetic repairs, not for major masonry movement. If you want an invisible finish in face brickwork, mortar repair is usually more natural-looking than sealant.

Step 5: Repoint cracked mortar joints

If the bricks are sound but the mortar joints are cracked or fretting, repointing is the proper repair. Mix a repair mortar compatible with the existing wall. For many general repairs, a mortar around 1:2:3 cement:lime:sand is suitable, but older homes may need a softer lime-rich mix to avoid damaging the bricks.

Dampen the joint and surrounding bricks so they do not suck moisture too quickly from the new mortar. The brickwork should be damp, not dripping wet.

Pack the mortar firmly into the joint in layers using a pointing trowel. Compact it properly to eliminate voids, then finish the joint to match the existing profile, such as ironed, flush or raked.

Allow the mortar to firm up before brushing off crumbs. Protect the repair from hot sun, wind and rain while it cures.

💡 Mortar that is too strong can cause old bricks to crack. Matching the original mortar hardness is just as important as matching the colour.

Step 6: Replace cracked or loose bricks

If a brick is badly split, drummy, loose or fractured through its body, replacing it is better than patching it.

Carefully cut out the mortar around the damaged brick using a grinder or plugging chisel. Break the brick inward in small pieces and remove it without disturbing surrounding masonry. Clean out the cavity fully.

Dampen the cavity and replacement brick. Butter the sides and bed of the new brick with fresh mortar, then slide it into place so it aligns with the surrounding courses and joint widths. Tool the joints to match the existing finish.

Check alignment with a straightedge and level before the mortar sets.

Step 7: Consider crack stitching only for engineered repairs

For recurring stepped cracks in masonry, some repairs use helical bars set into cut mortar joints with grout. This is commonly called crack stitching.

While repair kits are available, this should not be treated as a simple DIY fix when the wall is loadbearing or movement-related. The spacing, embedment depth, bar length and grout system should follow the manufacturer’s engineering details or a structural engineer’s specification.

As a rule, if you are considering stitching, it is time to get a professional assessment first.

Step 8: Cure and protect the repair

Fresh mortar needs controlled curing. Mist the repair lightly in warm or windy weather and protect it with plastic sheeting or damp hessian for at least 24–72 hours, depending on weather conditions.

Do not wash the wall aggressively straight after the repair. Let the mortar gain strength before any cleaning or painting.

Avoid heavy impact, drilling or pressure washing near the repair while it cures.

Step 9: Monitor the wall after repair

Once the repair is complete, keep an eye on the area over the next few months. Reopening cracks, fresh stair-step cracking, or movement near openings may mean the original cause has not been solved.

Check site drainage, leaking downpipes, garden beds built against the wall, nearby large trees and changes in ground moisture. Long-term crack control often depends on managing water and soil movement around the home.

Common Mistakes to Avoid

1.Repairing a structural crack without identifying the cause, such as footing movement or drainage issues.
2.Smearing mortar over the surface instead of raking out the joint to at least 15–20 mm depth.
3.Using mortar that is too strong for older brickwork, which can damage surrounding bricks.
4.Replacing or pointing bricks without dampening the area, causing the mortar to dry too fast and crack.
5.Ignoring active movement signs like widening cracks, bulging walls or sticking doors and windows.

Pro Tips

1.💡 Take a photo and measure the crack before starting, so you can tell later whether movement has continued.
2.💡 Match the mortar colour by making a small sample first and letting it dry fully before final use.
3.💡 For face brickwork, remove and replace failed mortar neatly rather than relying on surface fillers for a better visual result.
4.💡 Hire a quality angle grinder and dust extraction setup if you only have a few repairs to do; it is usually more economical than buying for one-off use.
5.💡 If several cracks appear after a dry summer or heavy rain period, get drainage and footing conditions checked before spending money on repeated patch repairs.

Recommended Tools

125 mm angle grinder with diamond masonry blade — ideal for raking out mortar joints cleanly
Brick bolster and club hammer — best for controlled brick removal and trimming
Pointing trowel set — useful for packing and finishing mortar joints accurately
Helical crack repair kit — only for use where an engineered or manufacturer-specified stitching repair is appropriate
Dust extractor or wet-cut attachment — reduces silica dust and improves safety

Frequently asked questions

How do you repair cracked mortar joints in brick walls?
Repair cracked mortar joints by raking out failed mortar to a depth of 15 to 20 millimetres using a plugging chisel or diamond raking blade. Clear dust completely, dampen the bricks, and firmly pack fresh mortar matching the original compressive class into the joint using a pointing trowel.
When is a crack in a brick wall considered structural?
A crack is considered structural when it exceeds 5 millimetres in width, forms a stepped diagonal pattern through the brick units themselves, or prevents doors and windows from operating smoothly. According to AS 2870, cracks wider than 5 millimetres fall into Damage Category 3 or higher, requiring professional engineering assessment.
What mortar mix ratio should be used for repointing Australian brickwork?
Use an M3 mortar mix of 1 part cement, 1 part hydrated lime, and 6 parts brickies sand for general external brickwork. For older, softer colonial bricks, an M2 mix of 1 part cement, 2 parts lime, and 9 parts sand prevents modern high-strength mortar from spalling historic masonry units.
Can you use flexible sealant instead of mortar to fix brick cracks?
Flexible polyurethane sealants such as Sikaflex-11FC can be used to seal articulation and control joints or temporary non-structural weather gaps. Rigid brickwork should generally be repointed with lime-cement mortar because elastomeric sealants prevent moisture breathability and do not restore masonry compressive strength or shear resistance across courses.
What safety equipment is legally required when grinding mortar joints?
Grinding out mortar requires an AS/NZS 1716-compliant P2 respirator or fitted M-class dust extraction system to prevent respirable crystalline silica inhalation under Safe Work Australia regulations. Certified eye protection, class 4 hearing protection, protective leather rigger gloves, and steel-capped safety boots are also mandatory on Australian worksites.