Skip to main content

How to Repair Rust on a Ute Tray

Repair ute tray rust by cutting out corrosion, welding matching steel and sealing both sides. Learn safe patching and when to call a qualified welder.

Quick answer

Repair ute tray rust by removing all corroded steel, fitting a patch that matches the original panel thickness, and welding it to sound metal. Seal the repair on both sides with compatible primer and coating. Repairs affecting mounts, crossmembers or other load-bearing parts need assessment against the vehicle maker’s procedure.

Skill level
Intermediate
Time
1-2 days, depending on rust severity
Trade
Welding & Fabrication
Updated
28 November 2026

Tools you will need

  • Unimig Viper 185 - Multi-Process MIG/TIG/Stick Welder
  • Milwaukee M18 FUEL 125mm - Angle Grinder
  • Speedglas 9100XX - Auto-Darkening Welding Helmet
  • Insize 1108-150 - 150mm Digital Vernier Caliper
  • Kincrome K12150 - Sheet Metal Aviation Snips Set
  • Sutton Tools 125mm - Polycarbide Rust Stripping Disc
  • U-POL Raptor - 2K Polyurethane Bed Liner Coating Kit

What is involved in repairing rust on a ute tray?

This guide will walk you through the process of repairing rust on a ute tray, focusing on common surface rust and small to medium-sized perforations. We'll cover preparation, cutting out the affected areas, fabricating and fitting new patches, and welding techniques to restore structural integrity and appearance. This project is suitable for those with basic welding experience or a willingness to learn.

What skill level is required for ute tray rust repair?

Intermediate — [Estimated time: 1-2 days, depending on rust severity]

What tools are essential for repairing rust on a ute tray?

MIG Welder (GMAW): 180-200 Amp capacity, capable of welding mild steel up to 6mm. (e.g., Lincoln Electric PowerMIG 210 MP, ESAB Rebel EMP 215ic). For welders over $1000, consider equipment finance options. Settings: Material Thickness (1.6mm sheet): Voltage: 17-19V, Wire Speed: 4-6 m/min Material Thickness (3mm sheet): Voltage: 19-21V, Wire Speed: 6-8 m/min Angle Grinder: 125mm (5-inch) with various discs: Cutting discs (1mm thin kerf) Flap discs (40-80 grit) Grinding discs (6mm thick) Plasma Cutter: (Optional, but highly recommended for clean cuts) 40-60 Amp capacity. (e.g., Everlast PowerPlasma 50S). Settings (1.6mm mild steel): Amperage: 25-35A, Air Pressure: 40-60 PSI (275-415 kPa) Drill: Cordless or corded, with various drill bits (3mm, 6mm, 8mm). Wire Brush: For grinder and hand use. Clamps: Vice grips, C-clamps, welding clamps. Sheet Metal Shears/Snips: For smaller, intricate cuts. Measuring Tape, Ruler, Scribe/Marker. Hammer and Dolly Set: For shaping and panel beating. Body Filler Applicators/Spreaders. Air Compressor: (If using plasma cutter or air tools).

What materials are needed for ute tray rust repair?

Mild Steel Sheet: 1.6mm and/or 3mm thick, depending on the original tray material and extent of repair. (e.g., 1200mm x 600mm sheet). MIG Welding Wire: 0.8mm ER70S-6 mild steel wire. Shielding Gas: Argon/CO2 mix (80% Argon / 20% CO2) – E.g., C25 or C20. (10L cylinder). Flow Rate: 10-12 L/min. Grinding Discs, Cutting Discs, Flap Discs: Replacements as needed. Rust Converter/Primer: Zinc-rich primer. Body Filler: Automotive grade. Paint: Matching automotive paint for topcoat. Thinners/Degreaser: For cleaning surfaces. Welding Anti-Spatter Spray.

Safety Requirements

ALWAYS wear an auto-darkening welding helmet (AS/NZS 1338.1 compliant). Wear leather welding gloves and a flame-retardant (FR) jacket or apron. Safety glasses (AS/NZS 1337.1) under your helmet and when grinding/cutting. Hearing protection (earplugs/earmuffs) when grinding or using loud tools. Steel-capped boots. Ensure adequate ventilation and fume extraction. Work in a well-ventilated area or use a fume extractor. Welding fumes can be hazardous. Fire Safety: Keep a fire extinguisher (ABC type) readily available. Remove all flammable materials from the work area. Have a fire watch/spotter if working in a confined space or near combustibles. Consider a hot work permit if required by local regulations. UV and Arc Flash Protection: Ensure bystanders are protected from welding arc flash with welding screens or by keeping them a safe distance away. AS/NZS 1554: For any load-bearing repairs, ensure your welding meets the requirements of AS/NZS 1554. This guide focuses on general repairs, but structural integrity is paramount.

Step-by-Step Guide

Step 1: Assess and Prepare the Area

Thoroughly clean the rusted area with a wire brush and degreaser to remove dirt, grease, and loose rust. Use a hammer to tap around the rust to identify weak spots and determine the full extent of the damage. Mark the areas to be cut out, ensuring you go beyond the visible rust into solid, healthy metal.

Step 2: Cut Out Rusted Sections

Using an angle grinder with a 1mm cutting disc or a plasma cutter, carefully cut out the marked rusted sections. Aim for straight lines and clean corners where possible, as this makes fabricating patches easier. For plasma cutting, maintain a consistent standoff distance and travel speed for a clean cut. Be mindful of any wiring or fuel lines underneath the tray. Remove all cut-out pieces.

Step 3: Fabricate New Patch Panels

Measure the dimensions of the holes you've cut out. Transfer these measurements to your new mild steel sheet (1.6mm or 3mm, matching the original tray thickness). Use a scribe and ruler for accuracy. Cut the new patch panels slightly larger than the holes (e.g., 5-10mm overlap) if you plan to butt weld, or precisely to fit if you're doing a flush repair. For curved sections, you may need to gently shape the patch using a hammer and dolly. Clean the edges of the new patches with a flap disc to remove any burrs or sharp edges.

Step 4: Prepare Edges for Welding

Grind a slight bevel (approx. 30-45 degrees) on the edges of both the existing tray metal and the new patch panels, especially for thicker materials (3mm+). This creates a "V" groove for better weld penetration. Clean all mating surfaces thoroughly with a flap disc to bright, shiny metal. This removes any paint, rust, or contaminants that could compromise the weld.

Step 5: Fit and Tack Weld Patch Panels

Position the new patch panel into the opening. Use clamps to hold it firmly in place, ensuring it's flush or slightly recessed if you plan to fill with body filler later. Begin tack welding the patch in place. Apply small, intermittent tacks (10-20mm long) every 50-75mm around the perimeter. Allow each tack to cool slightly before applying the next to minimise heat distortion. For MIG welding 1.6mm mild steel, start with Voltage: 17V, Wire Speed: 4.5 m/min.

Step 6: Weld the Patch Panels

Once the patch is securely tacked, begin welding the seams. Use a "stitch" welding technique (short welds, 20-30mm long, skipping around the patch) rather than a continuous bead. This helps to manage heat input and prevent warping. Allow the welds to cool between stitches. For MIG welding 1.6mm mild steel, use Voltage: 18V, Wire Speed: 5 m/min, Gas Flow: 10 L/min. For 3mm mild steel, use Voltage: 20V, Wire Speed: 7 m/min, Gas Flow: 12 L/min. Ensure good penetration without burning through.

Step 7: Grind and Finish Welds

Once all welding is complete and cooled, use an angle grinder with a grinding disc to carefully grind down the welds until they are flush with the surrounding metal. Switch to a flap disc (80 grit) to smooth out the ground areas and blend them into the original panel. Be careful not to remove too much parent metal.

Step 8: Apply Rust Protection and Finish

Clean the repaired area thoroughly with degreaser. Apply a rust converter or a zinc-rich primer to all bare metal surfaces, following the manufacturer's instructions. Once dry, apply automotive body filler if needed to achieve a perfectly smooth surface. Sand the filler smooth, then prime and paint the repaired area to match the rest of the ute tray.

Common Mistakes to Avoid

1.Not cutting out enough rust: Leaving even small specks of rust will lead to it returning quickly. Always cut into healthy metal.
2.Poor preparation: Failing to clean surfaces properly before welding results in weak, porous welds and contamination.
3.Overheating the panel: Continuous welding without allowing cooling time causes warping and distortion, making the repair look uneven.
4.Incorrect welder settings: Using too much heat can burn through thin material; too little results in poor penetration and weak welds.
5.Inadequate safety gear: Neglecting PPE can lead to serious injuries, including arc eye, burns, and respiratory issues.

Pro Tips

Practice on scrap: Before touching your ute, practice cutting and welding on similar thickness scrap metal to dial in your machine settings and technique. Use a magnet: A strong magnet can be used on the underside of the patch to help hold it flush while tacking, especially on larger, flat areas. Backing bar: For very thin material or difficult areas, a copper or aluminium backing bar behind the weld can help dissipate heat and prevent burn-through. Check for pinholes: After grinding, spray the area with a light coat of primer. Any pinholes will show up as dark spots, indicating areas that need re-welding and grinding. Consider a spot welder: For very thin sheet metal (under 1.2mm), a spot welder can provide a cleaner, less heat-intensive repair, but MIG is generally more versatile for ute trays.

Recommended Tools

1.Lincoln Electric PowerMIG 210 MP: A versatile multi-process welder, excellent for MIG, TIG, and Stick, making it a great all-rounder for various projects.
2.Everlast PowerPlasma 50S: A robust plasma cutter offering clean, fast cuts on various metals, significantly speeding up material preparation.
3.Metabo HPT (Hitachi) G13SR4 125mm Angle Grinder: Reliable and powerful for cutting, grinding, and flap disc work, a workshop staple.
4.Speedglas 9100XXi Auto-Darkening Welding Helmet: Top-tier optical clarity and comfort, crucial for long welding sessions and precise work.
5.Strong Hand Tools Adjust-O Magnet Squares: Invaluable for holding workpieces at precise angles for tacking and fit-up.

Frequently asked questions

Can you use body filler to repair rust on a ute tray?
No, body filler cannot replace rusted or perforated steel on a ute tray. Cut out the damaged metal and weld in a suitable steel patch; filler is only for a thin cosmetic skim over sound, prepared metal. Check the vehicle maker’s repair procedure if the damage affects a load-bearing area.
What thickness steel should I use to patch a ute tray?
Use steel that matches the original tray panel’s thickness and type; there is no single gauge suitable for every ute. Measure sound metal before cutting and check the manufacturer’s repair information. AS/NZS 1554.1 covers structural steel welding, but it is not a universal repair specification for vehicle body panels.
How far should I cut back rust on a steel ute tray?
Cut back until the remaining steel is clean, solid and free of scale, thinning and perforation. Rust can extend beneath paint or overlap seams, so inspect the area after exposing the metal rather than relying on a fixed extra margin. If corrosion reaches a crossmember, mount or chassis component, get a qualified assessment.
How do you stop a ute tray warping while welding a rust patch?
Limit heat input by making short, spaced welds and moving between sections instead of running a continuous bead. Clamp the patch securely, allow the metal to cool between welds and check its fit as you progress. The appropriate weld length and sequence depend on panel thickness and the joint design.
Should you disconnect the battery before welding a ute tray?
Yes, isolate the vehicle electrical system according to the manufacturer’s welding instructions before welding. Switch off the ignition, remove the key and disconnect the battery in the specified order; some vehicles also require electronic modules to be isolated. Attach the welder’s earth clamp close to the repair, on clean metal.
What coating should you use after repairing rust on a ute tray?
Use a coating system compatible with the prepared steel and the product maker’s instructions, and protect both sides of the repair. Apply the specified primer before a bed liner such as U-POL Raptor. Two-pack coatings may contain isocyanates; follow the safety data sheet and use suitable spray facilities and respiratory protection.

Written by Welder, the Welding & Fabrication specialist at VIC.Tools.